Introduction
We can supply customers with 3 kinds of corrosion resistant super-elastic alloy, including 3J1, 3J2 and 3J3. This alloy is of Fe-Ni-Cr austenite precipitation strengthening super-elastic alloy. After solid solution treatment, it is of good plasticity, low hardness and easy forming. High mechanical property and elastic property are obtained by aging treatment after solid solution or cold strain. This super-elastic alloy has features of high strength, high elasticity modulus, weak magnetic, good corrosion resistance, thermal stability, etc. It can work under higher temperature, larger stress or corrosive medium conditions.
3J1 can work at a temperature of below 250℃.
Based on the 3J1 alloy, 3J2 and 3J3 are formed by adding with 5% and 8% molybdenum. They have higher heat resistance, and the operating temperature is improved to 350℃ and 450℃ respectively. This series alloys can also be used at low temperature (such as near -200℃).
Supplied typesGrade | 3J1 | 3J2, 3J3 | ||||||
varieties | Cold rolled strip material | Cold drawn wire | Cold-drawn polished bar | Hot rolled rod | Forged material | Hot rolled flat material | Cold rolled strip material | Cold drawn wire |
Thickness and diameter (side length) (mm) | 0.05~3.5 | 0.10~6.0 | 3.0~30.0 | 3.0~25.0 | >5~100 | 4.0~13 | 0.07~2.0 | 0.1~5.0 |
Width (mm) | 50~250 | -- | -- | -- | -- | -- | 50~200 | -- |
Length (mm) | -- | -- | -- | ≤500 | ≤300 | ≥300 | -- | -- |
Grade | C | Mn | Si | P | S | Ni | Cr | Mo | Ti | Al | Fe |
3J1 | ≤0.05 | ≤1.00 | ≤0.80 | ≤0.020 | ≤0.020 | 34.5~36.5 | 11.5~13.0 | -- | 2.70~3.20 | 1.00~1.80 | Balance |
3J2 | ≤0.05 | 0.8~1.20 | ≤0.50 | ≤0.010 | ≤0.010 | 35.0~37.0 | 12.5~13.5 | 4.0~6.0 | 2.70~3.20 | 1.00~1.30 | Balance |
3J3 | ≤0.05 | 0.8~1.20 | ≤0.50 | ≤0.010 | ≤0.010 | 35.0~37.0 | 12.0~13.0 | 7.5~8.5 | 2.70~3.20 | 1.00~1.30 | Balance |
Grade | Varieties and requirements | Heat treatment process |
3J1 | Strip | Solid solution treatment at 920~950℃+ 2~4h aging treatment at 650~750℃, then naturally cooling in air or furnace |
Cold strain + 2~4h aging treatment at 600~700℃, then naturally cooling in air or furnace. | ||
Wire | Cold strain + 2~4h aging treatment at 500~700℃, then naturally cooling in air or furnace. | |
Bar | Cold strain + 2~4h aging treatment at 650~750℃, then naturally cooling in air or furnace. | |
Hot rolled/ forged | Solid solution treatment at 950~980℃+≥4h aging treatment at 700~750℃, then naturally cooling in air or furnace. | |
3J2 | Strip | Solid solution treatment at 970~1000℃+ 2-4h aging treatment at 700~750℃, then naturally cooling in air or furnace. |
Cold strain + 2~4h aging treatment at 650~750℃, then naturally cooling in air or furnace. | ||
Wire | Cold strain + 2~4h aging treatment at 630~700℃, then naturally cooling in air or furnace. | |
3J3 | Strip | Solid solution treatment at 1000~1050℃+ 2~4h aging treatment at 750℃, then naturally cooling in air or furnace |
Cold strain+2~4h aging treatment at 650~750℃, then naturally cooling in air or furnace | ||
Wire | Cold strain + 2~4h aging treatment at 600~700℃, then naturally cooling in air or furnace. |
Index
heat resistant alloy, cobalt alloy
OHMALLOY Material Co.,Ltd.
Office Add.: Room 311, No.1211, Mudanjiang Road, Baoshan, Shanghai
Factory Add.: No 126, Jincheng Road, Xindeng, Fuyang,Hangzhou City, Zhejiang Province
Tel.: +86-21-66796338
+86-21-66796337
Fax: +86-21-66796339